ASTM B424 Specification

Scope

This specification2 covers rolled nickel-iron-chromiummolybdenum-copper alloy (UNS N08825 and UNS N08221)* plate, sheet, and strip. 1.2 The values stated in inch-pound units are to be regarded as the standard. The values given in parentheses are for information only.

Chemical Composition

ElementUNS N08825UNS N08221
Nickel38.0 to 46.039.0 to 46.0
Chromium19.5 to 23.520.0 to 22.0
Iron22.0 minAbalance
Manganese1.0 max1.0 max
Carbon0.05 max0.025 max
Copper1.5 to 3.01.5 to 3.0
Silicon0.5 max0.5 max
Sulfur0.03 max0.03 max
Aluminum0.2 max0.2 max
Titanium0.6 to 1.20.6 to 1.0
Molybdenum2.5 to 3.55.0 to 6.5

Note :

A. Element shall be determined arithmetically by difference.

Mechanical Properties for Plate, Sheet, and Strip (All Thicknesses and Sizes Unless Otherwise Indicated)

AlloyConditionTensile Strength, min, ksi (MPa)Yield StrengthA (0.2 % Offset), min, ksi (MPa)Elongation in 2 in. or 50 mm (or 4 D), min, %
Hot-Rolled Plate:    
UNS N08825annealed85 (586)35 (241)30
UNS N08221annealed79 (544)34 (235)30
Cold-Rolled Plate:    
UNS N08825annealed85 (586)35 (241)30
UNS N08221annealed79 (544)34 (235)30
Hot-Rolled Sheet:    
UNS N08825annealed85 (586)35 (241)30
UNS N08221annealed79 (544)34 (235)30
Cold-Rolled Sheet:    
UNS N08825annealed85 (586)35 (241)30
UNS N08221annealed79 (544)34 (235)30
Cold-Rolled Strip:    
UNS N08825annealed85 (586)B35 (241)30B
UNS N08221annealed79 (544)B34 (235)30B

Note :

A. Yield strength requirements do not apply to material under 0.020 in. (0.51 mm) in thickness.
B. Not applicable for thickness under 0.010 in. (0.25 mm).